How Filler Particle Size and Shape Affect FCBGA Underfill

March 2026 CEO, COFA keypark@cofa.co.kr

A technical study of how the particle size distribution (PSD) and shape of filler particles affect underfill flow and void formation in fine-pitch semiconductor packaging such as Intel Foveros, TSMC CoWoS and HBM. As microbump pitch shrinks to a few tens of micrometers, filler design becomes a deciding factor in process success.

01 | Introduction

The fine-pitch packaging challenge

As semiconductor packaging moves to fine-pitch architectures such as Intel Foveros, TSMC CoWoS and HBM integration, the physical space inside the package is shrinking fast.

In these architectures, capillary underfill redistributes the thermo-mechanical stress between the silicon die and the substrate and improves mechanical reliability. But as microbump pitch falls to a few tens of micrometers, the path the underfill can flow through becomes more and more restricted.

The core problem

Under these conditions, the particle size distribution (PSD) and morphology of the filler inside the underfill directly affect flow behaviour and the tendency to form voids, and become deciding factors in whether the process succeeds.

Key trends in fine-pitch packaging

  • Intel Foveros: 3D stacking, microbump pitch < 50μm
  • TSMC CoWoS: Chip-on-Wafer-on-Substrate, ultra-high-density interconnect
  • HBM (High Bandwidth Memory): memory stacks requiring extremely fine pitch
  • Fan-out Wafer Level Package (FOWLP): finer redistribution layers (RDL)

These advances place new demands on underfill materials. Filler design in particular has to do more than tune thermo-mechanical properties: it must deliver both flowability and fill completion.

02 | Filler design

Why particle size distribution (PSD) matters

The size distribution of filler particles directly affects underfill flow resistance, viscosity and final fill quality.

Particle size and flow restriction

When the gap between microbumps narrows to 20-40μm in fine-pitch structures, whether filler particles can pass through that narrow channel becomes central to process success. If particles are too large relative to the gap, bridging occurs and blocks the flow.

Maximum particle size (D₉₀)

In fine-pitch structures, D₉₀ should be limited to one third of the gap or less to prevent bridging. Example: 30μm gap → D₉₀ ≤ 10μm

Median particle size (D₅₀)

D₅₀ sets the balance between viscosity and thermal conductivity. A range of 2-5μm generally suits fine-pitch applications.

Distribution width

A narrow PSD makes flow more predictable but can lower packing density. A broad PSD raises packing density but increases the risk from large particles.

Particle shape

Spherical particles flow well and carry a low bridging risk. Angular particles give higher mechanical properties but increase flow resistance.

Optimizing the particle size distribution

A bimodal PSD approach works well for fine-pitch applications. Small particles (1-3μm) secure flowability, while medium particles (5-8μm) improve mechanical properties and thermal conductivity.

Recommended PSD range (fine pitch)

D₁₀: 0.5-1.5μm | D₅₀: 2-5μm | D₉₀: 6-10μm
Shape: spherical, aspect ratio < 1.5

03 | Flow mechanism

Capillary flow and filler interaction

Capillary forces draw underfill into the gap between die and substrate. Along the way, filler particles create flow resistance and a filtering effect.

Capillary flow basics

Capillary flow speed is described by the Washburn equation:

v = (γ · cos θ · r) / (4η · L)

v: flow velocity | γ: surface tension | θ: contact angle | r: gap radius | η: viscosity | L: flow distance

How filler affects flow

  • Higher viscosity: adding filler raises underfill viscosity and slows the flow.
  • Shear thinning: a good underfill drops in viscosity under shear, which eases dispensing and flow.
  • Filtering: large filler particles collect at the entrance of a narrow gap and obstruct the flow.
  • Bridging: particles lock together in the gap and form a physical barrier that stops the flow entirely.

Design insight

In fine-pitch structures, lowering filler loading (40-55 wt%), keeping particles small (D₉₀ < gap/3) and using spherical particles raise the chance of a complete fill.

04 | Void formation

How voids form and how to prevent them

Voids are trapped air or unfilled areas left during underfilling, and they significantly reduce mechanical reliability.

Main causes of voids

1. Flow front imbalance

When underfill flows around the die in several directions, the flow fronts can meet near the center of the die and trap air. Uneven filler distribution makes this worse.

2. Filler bridging and filtering

When large filler particles block a narrow gap, underfill cannot reach some areas and voids remain. This happens most easily at the die center and corners.

3. Rising viscosity and onset of cure

If underfill viscosity rises during filling because of temperature or elapsed time, the flow slows or stops and leaves unfilled areas.

4. Trapped volatiles

Low-molecular-weight components or moisture in the underfill resin can vaporize during cure and form voids.

Void prevention strategies

Filler design

• Limit maximum particle size (D₉₀ < gap/3)
• Use spherical particles
• Narrow PSD to prevent bridging

Viscosity optimization

• Low initial viscosity (500-2,000 cP @ 25°C)
• Strong shear thinning
• Sufficient work life

Dispense pattern

• Four-side or multi-point dispensing
• Balanced flow fronts
• Vacuum or reduced-pressure environment

Process conditions

• Keep a low initial temperature (20-30°C)
• Appropriate preheat profile
• Two-step cure

High-risk structures for voids

• Large die (≥ 15×15mm)
• Ultra-fine pitch (< 30μm bump pitch)
• High I/O density (multi-row bump arrays)
• Complex die shapes (L-shaped, with cut-outs)

05 | Design guidelines

Filler design recommendations for fine pitch

Based on field experience and research, these are filler design guidelines for fine-pitch FCBGA underfill.

Parameter Recommended range Note
Bump pitch 20-40μm Ultra-fine-pitch applications
Filler D₉₀ ≤ 10μm One third of the gap or less
Filler D₅₀ 2-5μm Balance of flow and properties
Filler D₁₀ 0.5-1.5μm Fine particles to penetrate narrow gaps
Filler loading 40-55 wt% Lower loading recommended for fine pitch
Particle shape Spherical Aspect ratio < 1.5
Viscosity (25°C) 500-2,000 cP Shear thinning required
Work life (25°C) ≥ 4 hours Enough working time

Choosing the filler material

Silica (SiO₂) is the most widely used filler, with these advantages:

  • Improves thermal conductivity
  • Makes CTE easy to adjust
  • Chemically stable and low cost
  • Available in many particle sizes and shapes

For special applications, these fillers are also considered:

  • Alumina (Al₂O₃): when high thermal conductivity is required
  • Boron nitride (BN): electrical insulation with high thermal conductivity
  • Spherical silica: when the best possible flow is required

06 | Industry trends and technical requirements

The evolution of fine-pitch packaging and the underfill challenge

Semiconductor packaging keeps moving to finer pitch, and the technical demands on underfill materials are rising quickly with it.

Global packaging technology trends

The industry has steadily reduced interconnect pitch to improve performance and shrink size. The 40-50μm pitch common until the early 2020s is now shrinking below 30μm, and some leading-edge applications require ultra-fine pitch below 20μm.

Pitch reduction trend

2020: 40-50μm (mainstream HBM, flip-chip packages)
2023: 30-40μm (high-density flip chip, HBM2E/HBM3)
2025-2026: 20-30μm (next-generation HBM3E, 3D stacking)
Expected after 2028: 15μm or less (ultra-high-density interposers, linked to hybrid bonding)

Requirements by packaging architecture

1. HBM (High Bandwidth Memory)

HBM stacks memory dies vertically to maximize bandwidth and is currently the application where pitch is shrinking fastest.

  • HBM2E: 40μm pitch, underfill D₉₀ ≤ 12-15μm recommended
  • HBM3: 30-35μm pitch, underfill D₉₀ ≤ 10μm required
  • HBM3E (next generation): pitch 25μm or less, underfill D₉₀ ≤ 8μm required
  • Main challenges: stress management in multi-layer stacks, complete void-free fill

2. 3D-stacked flip chip (Intel Foveros and similar)

3D packaging that stacks dies vertically to integrate heterogeneous chips requires both ultra-fine pitch and low-stress design.

  • Current trend: 30-40μm pitch, ultra-low-stress underfill (modulus < 4 GPa)
  • After 2026: 20-25μm pitch, modulus target < 3 GPa
  • Main challenges: loss of properties from lower filler loading, securing flow through complex gap structures

3. TSMC CoWoS (Chip-on-Wafer-on-Substrate)

CoWoS uses ultra-high-density interposers and combines large dies with fine pitch, which makes underfilling harder.

  • Current: 35-45μm pitch, large dies (> 20×20mm)
  • Next-generation CoWoS-S/R: 25-30μm pitch, multi-chip integration
  • Main challenges: warpage control on large dies, viscosity control over long flow distances

4. Fan-Out Wafer Level Package (FOWLP)

FOWLP uses redistribution layers (RDL) to reach fine pitch without a substrate, and its thin package profile makes warpage control important.

  • Current trend: 40-60μm pitch, low-stress underfill
  • Next-generation eWLB: pitch 30μm or less, ultra-thin packages (< 0.5mm)
  • Main challenges: ultra-low CTE design, minimal warpage

Where filler technology is heading

As pitch narrows, the requirements on filler particle size and shape become stricter. The industry is developing filler technology in these directions:

Nano filler

Fillers with D₉₀ < 5μm for pitch below 15μm, combining nanoparticles (100-500nm) with submicron particles (0.5-2μm).

Better sphericity

Near-perfect spherical particles made by sol-gel or spray drying, reaching an aspect ratio < 1.2 to minimize flow resistance.

Surface treatment

Optimized silane coupling agents strengthen filler-resin adhesion and keep mechanical properties high even at low loading.

Hybrid filler systems

Combinations such as silica + alumina + BN, allowing thermal conductivity, CTE and modulus to be tuned independently.

Common industry challenges

As pitch falls below 25μm, underfills designed for 40-50μm pitch no longer work. New filler designs and new resin systems are urgently needed, with breakthroughs required in particular in:

  • Ultra-fine filler dispersion: preventing agglomeration of nanoparticles and dispersing them evenly
  • Low-viscosity resins: keeping reliability as filler loading drops
  • Wider process window: longer working time and a broader temperature range
  • Cost efficiency: lowering the cost of making nano fillers

07 | Conclusion

Key takeaways and recommendations

In fine-pitch FCBGA packaging, filler design decides whether the underfill process succeeds.

Main conclusions

  • Particle size is decisive: D₉₀ must stay at one third of the gap or less to prevent bridging.
  • Spherical particles are essential: particle shape strongly affects flow in fine-pitch structures, and spherical particles are the best choice.
  • Lower filler loading: loading in the 40-55 wt% range secures flow and fill completion.
  • Bimodal PSD works: small particles secure flow while medium particles provide the properties.
  • Process integration is required: filler design alone is not enough; dispense pattern, temperature control and cure profile must be optimized together.

Future research directions

  • Nano filler technology for ultra-fine pitch below 15μm
  • AI-based PSD optimization and flow simulation
  • Next-generation low-stress underfill for 3D stacking
  • Environmentally friendly filler materials and resin systems

Work with COFA on your fine-pitch challenge

COFA analyzes your package structure and process conditions and provides optimized filler design and underfill solutions. If voids, incomplete flow or reliability problems are holding back your fine-pitch packaging, contact us.

From sample evaluation to process optimization and custom material development, our packaging engineers support your project.

Technical inquiry